Influence of the Fe3O4/SiO2 ratio on the strength and fracture mechanisms of magnetite ore like materials under uniaxial compression

PLOS ONE
CC BY
이 매체는 공공·자유 라이선스로 본문을 직접 표시합니다.

Figures
Abstract
The Fe3O4/SiO2 ratio is an important compositional factor affecting the mechanical behavior of magnetite ore like materials. In this study, uniaxial compression simulations were carried out using particle flow models with different Fe3O4/SiO2 ratios, and the simulated crack evolution and acoustic emission (AE) responses were interpreted together with SEM-EDS observations. The uniaxial compressive strength varies non monotonically with the Fe3O4/SiO2 ratio. As the ratio decreased from 3.00 to 1.00, the peak strength decreased from 131.64 MPa to 81.95 MPa. Further decreases in the ratio to 0.60 and 0.33 increased the peak strength to 146.45 MPa and 151.01 MPa, respectively. At Fe3O4/SiO2 = 1.00, the heterogeneous mineral interfaces appeared highly connected, and cracks preferentially initiated and coalesced along weak SiO2-Fe3O4 and Fe3O4-Al2O3 contacts, producing through going failure paths and the lowest strength. In SiO2 rich specimens, strongly bonded contacts formed a more stable load bearing framework that arrested or deflected cracks and improved strength. Crack number evolution and AE results show that failure was dominated by tensile crack propagation, whereas shear and mixed mode events were mainly associated with late stage coalescence, local sliding, and failure zone formation. SEM-EDS observations provide qualitative microstructural support for this mechanism: Si rich regions tend to impede crack propagation, whereas Si-Fe intergrown regions promote crack linkage. The strength variation is therefore attributed to ratio dependent changes in mineral contact combinations, the continuity of the load bearing framework, and the connectivity of heterogeneous interfaces.
Citation: Yuan T, Yang T, Yang Z, Zhao Q, Zhao Y, Li J, et al. (2026) Influence of the Fe3O4/SiO2 ratio on the strength and fracture mechanisms of magnetite ore like materials under uniaxial compression. PLoS One 21(11): e0363600. https://doi.org/10.1371/journal.pone.0363600
Editor: Zihan Liu, The University of Hong Kong, HONG KONG
Received: September 18, 2026; Accepted: November 10, 2026; Published: November 24, 2026
Copyright: © 2026 Yuan et al. This is an open access article distributed under the terms of the Creative Commons Attribution License, which permits unrestricted use, distribution, and reproduction in any medium, provided the original author and source are credited.
Data Availability: All data underlying the findings of this study are available in the manuscript and its Supporting Information files.
Funding: This work was supported by the National Natural Science Foundation of China (No. 52374157), the Central Government Guides Local Science and Technology Development Fund (Grant No. 2026JH6/101000031), the Top-notch Young Talents of the Liaoning Revitalization Talent Program (Grant No. XLYC2503141), the Fundamental Research Funds for the Central Universities (N25BSS079) and the Fundamental Research Funds for the Central Universities (N25BSS082), the S&T Innovation and Development Project of Information Institution of Ministry of Emergency Management (Project No.2025509). The funders provided financial support for this research. The funders provided financial support for this research and were involved in the study design, data collection and analysis, decision to publish, and preparation of the manuscript.
Competing interests: The authors declare that they have no known financial interests or personal relationships that could have appeared to influence the work reported in this paper.
1. Introduction
Natural rocks and ores are heterogeneous aggregates composed of mineral phases with different physical and mechanical properties. Differences in hardness, elastic modulus, fracture toughness, and bonding behavior give rise to uneven load transfer and preferential fracture under external loading. Strong phases may form the main load bearing framework, whereas weak phases and heterogeneous mineral interfaces commonly generate local stress concentrations and provide favorable sites for microcrack initiation and propagation. In this study, Fe3O4, SiO2, and Al2O3 equivalent phases were used to represent the main iron bearing phase, siliceous gangue, and aluminous accessory component of magnetite ore, respectively. The Al2O3 equivalent phase content was kept constant, and the Fe3O4/SiO2 equivalent phase ratio was varied to examine its effect on uniaxial compressive strength, crack propagation, and AE characteristics. This work aims to clarify how load bearing framework transition and interfacial crack coalescence jointly control the macroscopic failure mode.
Research on the mechanical behavior of rocks and ores has gradually moved from macroscopic strength testing alone toward combined analyses of mineral composition, grain scale structure, and mesoscopic crack evolution. Du et al. [1] investigated mineral composition, grain size, and AE characteristics in various rocks and showed that mineral type and grain scale strongly affect strength, failure mode, and AE response. Zhang et al. [2] used the PFC-GBM method to examine the influence of mineral components on the uniaxial compressive behavior of granite, demonstrating that mineral volume fraction and contact type can alter crack propagation paths and fracture energy dissipation. He et al. [3] further showed, from a three dimensional perspective, that mineral heterogeneity and preexisting fissures influence UCS; mineral spatial distribution therefore affects both strength and crack coalescence patterns. Zhou et al. [4] reported that weak minerals can induce crack deflection, clustering, and coalescence, thereby modifying the overall failure mode of crystalline rocks. Hu et al. [5], Zhang et al. [6], and Liu et al. [7] investigated damage evolution in heterogeneous rocks using digital image based modeling, grain based FDEM, and grain block models, respectively. Their results show that realistic mineral structures, grain scale geometric heterogeneity, and contact heterogeneity are key factors in mesoscopic fracture development. The mechanical effect of mineral composition should be interpreted through mineral contact relationships, interface strength contrast, and crack propagation paths, rather than through the content of a single mineral phase alone.
PFC, DEM, GBM, and AE monitoring are widely used to study crack evolution and damage identification in rocks. Caulk [8] developed a DEM-AE simulation approach that accounts for rock heterogeneity and showed that DEM can be used to analyze AE event distributions and energy release in heterogeneous materials. Liu et al. [9] proposed a method for estimating the AE b value in rocks, providing a basis for identifying crack development stages from AE parameters. Ma et al. [10] simulated AE source mechanisms in Brazilian splitting tests using moment tensor inversion, showing that AE analysis can distinguish different crack types. Jing et al.[11] investigated the relationship between crack propagation and AE precursor characteristics through numerical simulation. Other studies have analyzed crack evolution and AE responses in jointed or fractured rock specimens under uniaxial compression [12–17]. Together, these studies show that crack number, crack type, AE activity, energy release, and spatial distribution can describe the failure process from local damage initiation to global instability. Recent reviews of DEM applications in mineral comminution also emphasize that particle scale contact laws, bond breakage, and calibration strategies are essential for linking microscopic particle interactions with macroscopic mineral breakage behavior [18].
In magnetite ore like materials, Fe3O4, SiO2, and Al2O3 bearing components generally correspond to the main iron bearing phase, siliceous gangue, and aluminous accessory phases, respectively. Changes in their relative proportions can alter the mineral framework, interfacial structure, and particle bonding state. Studies on magnetite hematite ores, iron ore pellets, high alumina iron ore fines, and sinter have shown that iron oxides, gangue minerals, impurity oxides, particle size, roasting conditions, and microstructure all affect ore structure and mechanical performance [19–26]. These studies confirm the importance of mineralogical variation in iron ore systems, but the role of mineral phase ratio in crack initiation and propagation in compressed magnetite ore like materials remains insufficiently resolved.
Although mineral heterogeneity, microscopic crack evolution, and AE responses have been widely discussed, most available studies focus on common rocks such as granite and sandstone, or on the metallurgical properties, sintering behavior, and beneficiation of iron ore. The mechanical response and fracture mechanism associated with changes in the relative contents of Fe3O4 and SiO2 equivalent phases in magnetite materials remain less well understood. In particular, it is still unclear how the Fe3O4/SiO2 equivalent phase ratio changes the proportion of strongly and weakly bonded contacts, the continuity of the load bearing framework, and the connectivity of cracks along heterogeneous interfaces. To address this issue, this study constructed a three phase mineral PFC model using Fe3O4, SiO2, and Al2O3 equivalent phases, hereafter denoted as Fe3O4, SiO2, and Al2O3. The Al2O3 equivalent phase content was kept constant, and the Fe3O4/SiO2 equivalent phase ratio was varied in uniaxial compression simulations. Crack initiation locations, crack type and crack number evolution, AE rupture types and magnitudes, and SEM-EDS microstructures were then analyzed to reveal how mineral phase ratio affects non monotonic strength variation, crack path selection, and macroscopic failure.
2. Material composition and numerical model
2.1. Parameter validation and establishment of the multi mineral particle model
Ore is a typical multi mineral composite, and its macroscopic mechanical behavior is controlled jointly by mineral composition, mineral content, and mineral interface characteristics. Before simulating specimens with different mineral phase ratios, the mineral composition of the tested ore was determined and the model parameters were validated. The parameter acquisition and validation procedure is summarized in Fig 1. The procedure includes open pit slope sampling, XRD mineral composition analysis, laboratory uniaxial compression testing, parameter assignment, and comparison between experimental and simulated results.
The schematic diagram was independently created by the research team, The illustration is provided for illustrative purposes only).
XRD testing was first conducted on core specimens collected from the mine slope to identify the main mineral components. The tested ore consists mainly of Fe3O4, SiO2, Al2O3, and minor accessory minerals. The XRD derived mass fractions of Fe3O4, SiO2, and the Al2O3 plus minor mineral group are 48.2 wt%, 33.3 wt%, and 18.5 wt%, respectively. On this basis, the specimen was simplified into three particle groups: Fe3O4, SiO2, and Al2O3. Fe3O4 and SiO2 represent magnetite and quartz, respectively, whereas Al2O3 was used as an equivalent phase for aluminosilicate minerals and other minor accessory phases.
Laboratory uniaxial compression tests were then performed on the core specimens to obtain the stress strain curve, peak strength, and failure mode. The mineral composition from XRD and the mechanical parameters from the uniaxial compression tests were introduced into the model. After calibration of the particle contact and parallel bond parameters, the simulated results agreed reasonably well with the experimental results. As shown in Fig 1, the experimental and simulated stress strain curves are similar in overall trend, peak strength level, and post peak stress drop behavior, and both show typical brittle failure. The stepwise fluctuations in the simulated curve arise mainly from discrete breakage of parallel bonds between particles, reflecting staged mesoscopic crack development. The simulated and experimental failure modes are also consistent: both show a main crack penetrating the specimen, local fragmentation in the lower part, and combined tensile shear failure. These comparisons indicate that the selected mesoscopic parameters can represent the basic mechanical response and fracture behavior of magnetite ore like materials under uniaxial compression.
The experimental and simulated peak strengths in Fig 1 are 100.90 MPa and 104.96 MPa, respectively. The simulated value is 4.06 MPa higher, giving a relative difference of (104.96 − 100.90)/100.90 × 100% = 4.02%. Calibration was assessed primarily by the peak strength and the slope of the approximately elastic portion of the stress strain curve, together with the overall curve shape and the main fracture pattern.
Using the validated parameters, multi mineral particle models with different Fe3O4/SiO2 ratios were established. The specimen was a two dimensional rectangle 50 mm wide and 100 mm high. Particles were generated with a random spatial distribution, radii of 0.35–0.525 mm, and an initial porosity of 0.10. The densities of SiO2, Fe3O4, and Al2O3 particles were set to 2320, 5200, and 3950 kg/m3, respectively. Particle contacts were represented by the parallel bond model. Different mesoscopic parameters were assigned to homogeneous mineral contacts and heterogeneous mineral interfaces to reflect differences in load bearing and fracture behavior among contact types. Strong and weak contacts are distinguished here by the relative tensile strength and cohesion assigned to the parallel bonds. Their elastic response is governed separately by the effective modulus and the normal to shear stiffness ratio.
To examine the effect of the Fe3O4/SiO2 ratio on strength and failure mechanism, the Al2O3 equivalent phase area fraction was fixed at 20%, and the relative contents of Fe3O4 and SiO2 were varied to generate six specimen groups, as listed in Table 1. This design represents a compositional transition from Fe3O4 rich to SiO2 rich ore and provides the basis for analyzing load bearing framework formation, interfacial crack propagation, AE response, and final failure mode.
The mineral percentages in Table 1 are the particle area fractions specified through the three volume fraction bins of the ball distribute command in the two dimensional model. The Fe3O4/SiO2 ratio is obtained by dividing the Fe3O4 area fraction by the SiO2 area fraction; for example, 50% Fe3O4 and 30% SiO2 give a ratio of 1.67. The measured accessory mineral content of 18.5 wt% was used as a compositional reference when selecting a fixed 20% particle area fraction for the Al2O3 equivalent phase in the composition series. This setting keeps the accessory component constant while Fe3O4 and SiO2 are exchanged within the remaining 80%, so that their relative proportion can be examined under a common accessory phase setting.
2.2. Acoustic emission simulation method
An AE monitoring method based on the parallel bonded particle model was established to relate mesoscopic damage evolution to AE response. In DEM simulations, breakage of a parallel bond between particles can be treated as a microcrack event. Microcrack events that are close in both time and space can be grouped into one AE event. By recording the position and time of parallel bond breakage, contact force variation, and relative particle displacement during loading, the location, number, magnitude, and rupture type of AE events can be obtained. These parameters characterize the damage process from local crack initiation and propagation to macroscopic coalescence. Because AE and microseismic monitoring share similar source location principles, reviews of microseismic source location techniques in underground mining provide useful support for interpreting the spatial distribution of simulated AE events [27].
In PFC based AE simulation, common characterization approaches include kinetic energy, strain energy, and moment tensor methods. Kinetic energy and strain energy methods can describe energy release, but they cannot directly distinguish tensile, shear, and mixed mode rupture. Magnitudes estimated from kinetic energy may also depend on the numerical energy dissipation scheme. The moment tensor method was therefore adopted here to establish the AE monitoring system and identify rupture mechanisms associated with particle bond failure under different mineral phase ratios [28].
During uniaxial compression, parallel bond breakage changes the force state and relative displacement of the particles at the two ends of the broken contact and causes redistribution of surrounding contact forces. This local mechanical response can be represented by the moment tensor of the AE source region. The bond break process was monitored in real time using the built in FISH language in PFC. For a single bond break event, the crack center was taken as the microcrack location. When several bond break events occurred continuously within a specified time interval and spatial neighborhood, they were grouped into the same AE hit, and the average position of their geometric centers was used as the AE source center. For each AE event, the moment tensor was calculated from the contact force variation around the fractured region and the position of each contact point relative to the source center, as expressed in Eq. (1):
(1)where represents the i-th component of the change in contact force between particles; and the j-th component of the distance between the contact point and the center of the source region.
To reduce computational cost and improve simulation efficiency, the complete evolution of the moment tensor was not stored at every time step. Instead, after an acoustic emission event was formed, only the scalar moment corresponding to the maximum moment tensor state was recorded. The scalar moment M0 can be calculated from the eigenvalues of the moment tensor, as given in Eq. (2):
(2)where is the j-th eigenvalue of the moment tensor matrix.
The magnitude of the acoustic emission event is calculated according to the scalar moment tensor of the event using the following Eq. (3) [28]:
(3)The magnitude defined by Eq. (3) is a logarithmic measure of scalar moment. Scalar moment combines the contact force changes and their distances from the source center, and therefore characterizes the size and intensity of the simulated rupture event. Larger magnitudes correspond to larger scalar moments. Released energy also depends on rupture displacement and stress change; the magnitude distribution is used here to compare relative event size and rupture intensity.
To identify the rupture mechanism of acoustic emission events, the moment tensor was decomposed into the sum of an isotropic component, a double couple component, and a compensated linear vector dipole component [29,30], as expressed in Eq. (4):
(4)where represents the isotropic component of the tensor, which serves as the center of expansion (or compression) and describes the volume change in the source region; the pure dipole component; and the compensatory linear vector dipole component.
Based on tensor monitoring results from deep laboratory experiments, fractures in the surrounding rock, and the direction of in situ stresses, Feignier proposed criteria for determining rock failure types [31]. Eq. (5) is used to identify the rock failure mechanism.
(5)where represents the eigenvalue of the deviatoric tensor and the tensor’s trace, while represents the volume change of the source. Feignier proposed that seismic events with R > 30% correspond to extensional failure, those with −30% ≤ R ≤ 30% correspond to shear failure, and those with R <−30% correspond to compressive failure [31], as shown in Fig 2 [32].
With this method, the number, magnitude, spatial distribution, and rupture type proportions of AE events were recorded during uniaxial compression. The AE responses were then compared with the stress strain curves, crack number evolution, and final failure patterns. This comparison helps clarify the relationships among mineral interface crack initiation, crack propagation, local fragmentation, and macroscopic coalescence under different Fe3O4/SiO2 ratios, and provides a numerical basis for analyzing damage evolution controlled by strong and weak contacts.
3. Uniaxial compression mechanical response
3.1. Characteristics of stress strain curve
Fig 3 shows the uniaxial compressive stress strain curves of specimens with different Fe3O4/SiO2 ratios. All six groups exhibit typical brittle deformation and failure during loading. Their stress strain responses include initial compaction, approximately elastic deformation, crack propagation, peak failure, and post peak stress drop. In the early loading stage, stress increases gradually with strain and the curve slope rises, reflecting compaction of particle contacts and adjustment of initial pores and locally unstable contacts. The curves then enter a relatively stable rising stage with an approximately linear stress strain relationship. At this stage, the external load is mainly carried by particle contacts and parallel bonds, and specimen deformation is predominantly elastic.
With increasing axial strain, local fluctuations or slight stress drops appear in the curves. These features correspond to local parallel bond breakage and the initiation and propagation of microcracks. The cracks have not yet formed a through going failure plane, so the specimen can still sustain additional load. The fluctuation intensity differs among the curves, showing that mineral composition affects the timing and development of mesoscopic contact failure. In the Fe3O4/SiO2 = 1.00 specimen, the pre peak fluctuations are more pronounced and the overall stress level is lower. This response reflects the higher development of heterogeneous mineral interfaces when Fe3O4 and SiO2 contents are similar. These local weak interfaces are more susceptible to damage, which reduces the stability of stress increase. By contrast, the Fe3O4/SiO2 = 0.33 and 0.60 specimens maintain higher pre peak stress growth, implying that higher SiO2 content helps form a relatively stable load bearing structure that suppresses early crack propagation.
Peak strength varies markedly with the Fe3O4/SiO2 ratio, As shown in Table 2. The Fe3O4/SiO2 = 0.33 and 0.60 specimens have the highest peak stresses, approximately 151.01 MPa and 146.45 MPa, respectively. The Fe3O4/SiO2 = 3.00 and 2.20 specimens show intermediate peak stresses of approximately 131.64 MPa and 127.81 MPa, respectively, while the Fe3O4/SiO2 = 1.67 specimen has a lower peak stress of approximately 112.61 MPa. The lowest peak stress, approximately 81.95 MPa, occurs at Fe3O4/SiO2 = 1.00. Thus, strength does not change monotonically with the Fe3O4/SiO2 ratio but reaches a clear minimum near Fe3O4/SiO2 = 1.00. This behavior suggests that macroscopic strength is governed by mineral spatial distribution, contact type proportions, and the coalescence capacity of heterogeneous interfaces, rather than by Fe3O4 or SiO2 content alone.
Peak strain and post peak curve shape also differ among the specimens. The Fe3O4/SiO2 = 0.33 and 0.60 specimens reach peak stress at relatively large strain levels and then undergo rapid post peak stress drops. These specimens can accumulate high load bearing capacity before peak failure, but once the main crack forms, global instability develops abruptly. The Fe3O4/SiO2 = 3.00 specimen also has relatively high peak strength, but its peak strain is smaller and its post peak stress drops rapidly, indicating stronger brittleness at high Fe3O4 content. The Fe3O4/SiO2 = 1.00 specimen combines low peak strength with pronounced pre peak fluctuations, implying earlier crack initiation and more progressive crack development at a relatively low stress level.
3.2. Preliminary assessment of the non monotonic strength variation
The stress strain curves and strength data show that specimen strength does not vary linearly with either Fe3O4 or SiO2 content. Instead, a pronounced minimum appears near Fe3O4/SiO2 = 1.00. Rock mechanical properties are affected by mineral composition, mechanical contrast among mineral phases, spatial distribution, and mineral boundary properties [33]. The strength minimum observed here is interpreted as the result of competition between a strongly bonded load bearing framework and crack coalescence along weak interfaces.
Under SiO2 rich conditions, strong contacts such as SiO2-SiO2, SiO2-Al2O3, and Al2O3-Al2O3 are more likely to form a continuous load bearing framework, which arrests, deflects, and forces weak interface cracks to bypass strong bonded regions. As a result, the specimen strength is relatively high. Previous studies have also reported that hard mineral grains or mineral grains with a high elastic modulus can induce crack deflection or crack arrest [34,35]. When Fe3O4/SiO2 approaches 1.00, the contents of Fe3O4 and SiO2 are close, and heterogeneous interfaces appear most developed. Cracks are more likely to initiate, propagate, and coalesce along weak interfaces such as SiO2-Fe3O4 and Fe3O4-Al2O3 contacts, leading to specimen instability at a relatively low stress level. This is consistent with GBM studies showing that mineral boundary parameters control crack evolution [36].
As Fe3O4 content increases further, the model gradually becomes Fe3O4 rich. The continuous coalescence capacity of heterogeneous interfaces may decrease, and crack propagation is no longer controlled by a global weak interface network. Strength therefore recovers to some extent. However, because Fe3O4 related contacts are weaker than SiO2/Al2O3 related strong contacts, Fe3O4 rich specimens still have lower load bearing capacity than SiO2 rich specimens. Fig 4 summarizes the effects of strongly bonded regions and weak contacts on crack deflection, interruption, and coalescence.
4. Crack evolution and acoustic emission response
4.1. Failure modes and AE event localization under different Fe3O4/SiO2 ratios
Fig 5 shows the final failure modes and AE event locations of specimens with different Fe3O4/SiO2 ratios. All six specimens show brittle failure under uniaxial compression, but the main crack position, crack coalescence pattern, degree of local fragmentation, and AE event distribution vary clearly with mineral ratio. AE events are concentrated near main crack zones, crack deflection regions, mineral boundaries, and local fragmentation zones rather than being randomly distributed. This distribution shows that AE localization captures crack initiation, propagation, and coalescence effectively.
The SiO2 rich specimens, Fe3O4/SiO2 = 0.33 and 0.60, have relatively high strengths and show localized splitting shear failure. Their main cracks and AE events are concentrated mainly in the middle lower parts of the specimens and near local mineral boundaries, instead of extending continuously throughout the specimens. Failure occurs after local damage has accumulated, followed by rapid post peak instability.
At Fe3O4/SiO2 = 1.00, the specimen has the lowest peak strength and a distinct failure pattern. In Fig 5(c), AE events are distributed more continuously along the main crack zone, indicating progressive damage accumulation along weak interfaces during loading. This pattern corresponds to tensile shear failure controlled by interface coalescence.
For the Fe3O4 rich specimens, Fe3O4/SiO2 = 1.67, 2.20, and 3.00, strength recovers relative to the Fe3O4/SiO2 = 1.00 specimen, but failure remains localized. Cracks develop mainly in local Fe3O4 related weak contacts and multi mineral boundary regions, with AE events concentrated near local main cracks, inclined cracks, and bottom fragmentation zones.
4.2. Crack initiation and propagation controlled by strong and weak contacts
Fig 6 shows crack initiation locations and enlarged local views of specimens with different Fe3O4/SiO2 ratios. Blue, green, and red particles represent SiO2, Fe3O4, and Al2O3, respectively, and the yellow boxes mark early crack initiation regions. Early cracks are concentrated near mineral boundaries, local multi mineral mixed regions, specimen edges, and Fe3O4 related weak contacts. Crack initiation is therefore strongly controlled by mineral contact type and bonding strength. The enlarged views further show that cracks mostly occur near heterogeneous contacts such as SiO2-Fe3O4 and Fe3O4-Al2O3, rather than directly penetrating continuous SiO2 rich regions or Al2O3 related strongly bonded zones. Stiffness, strength, and deformation mismatch at heterogeneous interfaces readily induce local stress concentration under compression. By contrast, strong contacts such as SiO2-SiO2, SiO2-Al2O3, and Al2O3-Al2O3 tend to arrest, deflect, or redirect cracks around these regions.
Previous studies have shown that rock microcracks can be classified as grain boundary, intragranular, intergranular, and transgranular cracks, and that mineral heterogeneity, boundary stress concentration, and elastic mismatch affect crack initiation and propagation paths [37]. The present results are consistent with these observations.
Fig 7 shows that cracks do not always continue along their initial direction. When they encounter strongly bonded mineral assemblages, their paths are interrupted, deflected, or diverted around strong zones, as seen in several yellow marked regions. Strongly bonded regions inhibit crack propagation by increasing local contact strength and changing stress transfer near the crack tip. Fe3O4 related weak contacts and SiO2-Fe3O4 heterogeneous interfaces, in contrast, provide preferential paths for further crack growth. The observed crack pattern is consistent with strong bond arrest and weak interface repropagation.
The yellow boxed regions in Fig 7(d) and 7(e) contain local interruptions of the crack traces beside the adjoining mineral assemblages. In Fig 7(f), the upper arrow identifies a change in crack direction, whereas the lower boxed region shows continued cracking through the adjacent contact zone. The interrupted traces support a local blocking effect of strongly bonded regions. Here, the arrest interpretation refers to the interruption visible in the plotted configuration.
4.3. Evolution of crack type and crack number
Fig 8 shows the evolution of ring count, total crack number, tensile crack number, and shear crack number with axial strain under different Fe3O4/SiO2 ratios. The total and tensile crack numbers are plotted on a × 103 scale, whereas the shear crack number uses an independent axis. The visual proximity of the curves does not mean that their absolute values are the same.
On the right, the axis nearest the plot gives total crack count (×103), the middle axis gives shear crack count, and the outermost axis gives tensile crack count (×103). Each curve should be read against its corresponding axis).
In all six specimens, the total crack number and tensile crack number follow highly similar trends, and tensile cracks are far more numerous than shear cracks. Crack multiplication during uniaxial compression is therefore controlled mainly by tensile cracking, consistent with the axial splitting and main crack coalescence observed in the failure mode analysis. Shear cracks are fewer but usually grow stepwise in the middle and late loading stages. They do not dominate initial cracking; instead, they contribute to crack linkage, local sliding, and final failure zone formation. The failure process is therefore tensile dominated tensile shear failure, with shear cracking mainly assisting late stage coalescence.
Macroscopic compression can produce local tensile stress because the contact forces are distributed among particles with different orientations. Lateral deformation and particle rotation also generate bending moments at bonded contacts. Consequently, the edge of a parallel bond can experience tensile stress even when its average normal force is compressive. The parallel bond model records tensile failure when the maximum tensile stress at the bond edge exceeds the tensile strength limit. If the bond remains intact, its shear stress is checked against the shear strength limit determined by cohesion, friction angle, and normal stress. This local criterion explains the predominance of tensile cracks under the applied compressive loading.
The influence of a shear crack depends on its position as well as its number. A shear failure near a crack intersection or an inclined damaged segment can link neighboring tensile cracks and allow local sliding, helping to form a continuous failure zone. Shear event markers beside tensile event clusters in the enlarged views of Fig 9(a), 9(b), 9(e), and 9(f) support this interpretation. Their spatial positions complement the stepwise increase in shear cracks in Fig 8 during the middle and late loading stages. Fig 8 counts broken bonds, while Fig 9 classifies AE events grouped from bond failures.
The crack growth rhythm changes with the Fe3O4/SiO2 ratio. In SiO2 rich specimens, crack number increases slowly during early loading and rises sharply near failure. In the Fe3O4/SiO2 = 1.00 specimen, cracks begin to increase at a lower strain level and grow more continuously. In Fe3O4 rich specimens, crack evolution generally shows slow early growth, stepwise middle stage propagation, and rapid late stage increase.
Ring count agrees well with crack number evolution. During early loading, the ring count remains low because few microcracks are generated and crack propagation is restricted. In the middle loading stage, discrete ring count peaks correspond to intermittent local crack propagation. Near failure, ring count increases sharply and synchronizes with the rapid growth of total and tensile cracks. This marks the transition from localized crack propagation to rapid crack coalescence and intensified fracture activity.
4.4. AE rupture types and spatial magnitude distribution
Fig 9 shows the distribution of AE rupture types and enlarged local views under different Fe3O4/SiO2 ratios. Blue, green, and red particles represent SiO2, Fe3O4, and Al2O3, respectively. Dark brown, pink, and yellow markers denote tensile, shear, and mixed mode rupture events. Tensile events dominate in all six specimens and are distributed mainly along the main fracture zones, confirming that crack propagation under uniaxial compression is primarily tensile. This observation agrees with the similar evolution trends of total and tensile crack numbers discussed above.
Although shear events are fewer, their locations are important. They occur mainly in crack deflection zones, inclined crack segments, crack intersections, and bottom fragmentation regions, showing that shear failure contributes to late stage crack linkage, local sliding, and failure zone formation rather than to initial cracking. Mixed mode events commonly appear near crack branching, deflection, and multi mineral intergrowth contacts, where tensile opening and shear displacement coexist. Tensile rupture controls crack initiation and main crack growth, shear rupture promotes linkage and local instability, and mixed mode rupture reflects combined failure near heterogeneous mineral interfaces. The Fe3O4/SiO2 ratio also changes the clustering pattern of rupture events. In SiO2 rich specimens, rupture events are mainly localized in main fracture zones and lower fragmentation regions. At Fe3O4/SiO2 = 1.00, tensile events are distributed more continuously along the main fracture zone and multi mineral interfaces, consistent with easier weak interface coalescence. In Fe3O4 rich specimens, rupture events concentrate near Fe3O4 related weak contacts and mineral boundaries.
Fig 10 shows the spatial distribution of AE magnitude under different Fe3O4/SiO2 ratios. The magnitude fields are highly heterogeneous. Low and medium magnitude regions form the main background, whereas high magnitude events concentrate near main crack propagation zones, crack deflection regions, crack intersections, and local fragmentation zones. High magnitude events are closely related to rapid crack growth, local sliding, and failure zone formation. In terms of rupture intensity, abundant tensile events correspond to continuous crack propagation, whereas localized shear and mixed mode events indicate stronger failure localization. In SiO2 rich specimens, high magnitude events mainly appear in late stage local fragmentation zones. At Fe3O4/SiO2 = 1.00, low to medium magnitude background regions coexist with local high magnitude patches, reflecting continuous damage accumulation along weak interfaces. In Fe3O4 rich specimens, high magnitude events are concentrated along local main fracture zones and weakened regions, indicating that larger AE events are associated with localized weak zones.
4.5. SEM-EDS observations supporting the crack propagation mechanism
Representative SEM-EDS images were used to further examine the crack initiation, propagation, and arrest mechanisms obtained from the PFC simulations. Fig 11 shows the relationship between mineral phase distribution and microcrack morphology. Green, pink, and yellow represent Si bearing, Fe bearing, and Al bearing phases, respectively. Instead of discussing the six Fe3O4/SiO2 ratios one by one, typical microscopic morphologies are used to examine how mineral rich regions and heterogeneous mineral contact zones influence crack paths and to provide qualitative support for the proposed mechanism weak interface initiation, strong bond arrest, and crack deflection or repropagation.
Fig 11 shows SEM-EDS characterized microcrack morphologies in regions with different mineral phase distributions. Continuous Si bearing regions or homogeneous mineral rich regions remain relatively intact, and no obvious through going microcracks are observed. These regions can impede crack propagation, and cracks do not readily penetrate continuous strongly bonded regions. By contrast, where Si bearing and Fe bearing phases are intergrown, cracks are more likely to propagate and link along heterogeneous mineral interfaces, showing a clear interface controlled feature. This behavior is attributed to compositional, stiffness, and strength contrasts between mineral phases, which induce stress concentration and deformation incompatibility near interfaces during loading and promote microcrack propagation along weakly bonded interfaces.
No large scale through going cracks are observed within Fe bearing phase rich regions. Crack propagation does not simply increase with increasing Fe bearing phase content. When one mineral phase becomes dominant, the overall connectivity of heterogeneous interfaces may decrease, and cracks are more likely to develop near local weak contacts or mineral boundaries. Local morphology also shows that cracks initiate and propagate near heterogeneous mineral contacts but tend to arrest, deflect, or become restricted after entering continuous homogeneous mineral regions or strongly bonded zones. This observation provides qualitative support for the crack arresting effect of strongly bonded regions.
The SEM-EDS observations support the crack path selection mechanism proposed above. Continuous Si bearing regions and homogeneous strongly bonded regions inhibit crack propagation, whereas heterogeneous interfaces with intergrown Si bearing and Fe bearing phases provide preferential channels for crack initiation and coalescence. Failure in Fe bearing phase rich regions is more strongly controlled by local weak interfaces and mineral boundaries. The strength differences caused by different mineral phase ratios are closely related to mineral spatial distribution, heterogeneous interface connectivity, and the crack arresting effect of strongly bonded regions. At the microscale, the SEM-EDS results are consistent with the non monotonic strength variation mechanism obtained from the PFC simulations.
5. Discussion
Previous studies have shown that mineral heterogeneity, mineral spatial distribution, and contact parameter differences can strongly affect the strength, crack propagation, and AE response of crystalline rocks. Hofmann et al. [38] used the GBM method to analyze the effects of mineral size, spatial distribution, and model discretization on the strength, elastic behavior, and microcrack development of granite. Zhang et al. [39] investigated the control of contact heterogeneity on granite fracture patterns, AE evolution, and energy release using PFC3D-GBM and AE-MT inversion. Zhao et al. [40] discussed asynchronous fracturing of different mineral phases in heterogeneous granite at the mineral scale. These studies provide an important basis for understanding the role of mineral heterogeneity in rock fracture. Recent reviews on macro meso mechanical behavior and damage mechanisms of rock related composite structures also highlight the association between macroscopic strength degradation, mesoscopic damage accumulation, interfacial interaction, and cooperative load bearing [41]. Liang et al. [42] described how tensile fractures and secondary interlayer shear fractures coalesce into a continuous failure boundary during the transition from open pit to underground mining. Li et al.[43] investigated how the layer thickness ratio affects shear creep induced strength degradation and progressive failure in soft hard interbedded rock masses.
This study focuses on magnetite ore like materials and varies the Fe3O4/SiO2 ratio while keeping the Al2O3 content constant. The results show that strength does not vary monotonically with either Fe3O4 or SiO2 content. A pronounced strength minimum occurs near Fe3O4/SiO2 = 1.00, where heterogeneous weak interfaces are most favorable for crack coalescence. The combined PFC, AE, and SEM-EDS results indicate that this behavior is governed by competition between the strongly bonded load bearing framework and the weak interface network. Under SiO2 rich conditions, the strongly bonded framework arrests or deflects cracks. At Fe3O4/SiO2 = 1.00, heterogeneous weak interfaces coalesce continuously. Under Fe3O4 rich conditions, failure is controlled mainly by localized weak zones. The three phase particle model used here remains a simplification of natural magnetite ore: mineral morphology, spatial intergrowth, and interfacial bonding are represented mainly by particle proportions and contact parameter differences. The observed non monotonic strength variation is therefore most appropriate for explaining the mesoscopic fracture mechanism of the Fe3O4、SiO2、Al2O3 three phase system and should not be generalized directly to all natural magnetite ores.
The strength of an individual contact determines the local threshold for bond breakage, while specimen failure also depends on whether damaged contacts can join into a continuous fracture path. This distinction helps explain the strength recovery on the Fe3O4 rich side. In Fig 5(c), the ratio 1.00 specimen shows a comparatively continuous concentration of damage and AE events along its principal fracture zone. The Fe3O4 rich specimens in Fig 5(d)–5(f) show more localized fracture activity. Local failure at weak Fe3O4 related contacts can therefore occur while neighboring intact contacts continue to transfer load. The resulting redistribution and localization of damage may delay the formation of a specimen spanning failure path and permit a higher peak load.
The two dimensional model captures in plane bond breakage, crack deflection, and the interaction of local fracture zones with mineral contact arrangements. In natural ore, out of plane contacts provide additional load transfer routes, and three dimensional cracks can develop around a mineral region through paths outside the modeled plane. These effects can change crack connectivity and the degree of localization. The present model therefore provides a basis for interpreting the in plane fracture mechanisms associated with composition changes, while three dimensional modeling would extend the analysis to spatial crack surfaces and load transfer. At the slope scale, Li et al. [44] combined UAV derived three dimensional geometry, structural discontinuity identification, and numerical simulation to investigate excavation induced failure.
Future work should focus on three aspects. First, repeated simulations with multiple random seeds are needed to evaluate the variability of peak strength, crack initiation stress, crack number, and failure mode, and to test the stability of the observed strength minimum. Second, the mineral types of the particles at both ends of each bond break event should be exported so that fracture proportions of different contact types can be quantified. This would allow the weak interface initiation and strong bond arrest mechanisms to be tested directly at the contact scale. Third, energy evolution analysis should be incorporated. Together with three dimensional PFC modeling, CT or SEM-EDS based image reconstruction, and laboratory uniaxial compression tests with AE monitoring and fracture surface observations, this analysis would provide a more complete validation of the proposed competition mechanism between strongly and weakly bonded contacts.
6. Conclusion
In this study, a three phase mineral particle model with fixed Al2O3 content and varying Fe3O4/SiO2 ratios was constructed using PFC. The uniaxial compressive strength, failure mode, crack evolution, AE response, and SEM-EDS microfracture morphology of specimens with different mineral phase ratios were analyzed. The main conclusions are as follows:
- (1) The Fe3O4/SiO2 ratio significantly affects the uniaxial compressive strength of the specimens, and the strength variation is non monotonic. As the Fe3O4/SiO2 ratio decreases from 3.00 to 1.00, peak strength decreases and reaches a minimum of 81.95 MPa at Fe3O4/SiO2 = 1.00. When the ratio decreases further to 0.60 and 0.33, peak strength increases to 146.45 MPa and 151.01 MPa, respectively. Specimen strength is controlled by mineral contact type, strongly and weakly bonded structures, and heterogeneous interface connectivity, rather than by Fe3O4 or SiO2 content alone.
- (2) The low strength of the Fe3O4/SiO2 = 1.00 specimen is mainly caused by through going failure along heterogeneous interfaces. At this ratio, Fe3O4 and SiO2 contents are similar, and heterogeneous contacts such as SiO2-Fe3O4 and Fe3O4-Al2O3 contacts are more developed. Cracks therefore initiate, propagate, and coalesce more easily along weak interfaces, forming continuous failure channels. In SiO2 rich specimens, strongly bonded contacts such as SiO2-SiO2, SiO2-Al2O3, and Al2O3-Al2O3 contacts are more likely to form a load bearing framework that arrests, deflects, and redirects cracks, thereby improving specimen strength.
- (3) Crack evolution and AE results show that failure in all six specimens is dominated by tensile crack propagation. Shear cracks and mixed mode ruptures mainly contribute to late stage crack linkage, local sliding, and failure zone formation. The total crack number and tensile crack number have highly consistent evolution trends. Ring count and magnitude contours show that rapid crack multiplication and enhanced AE activity are concentrated along main fracture zones, crack deflection regions, crack intersection regions, and local fragmentation zones. Crack patterns under different mineral phase ratios can be interpreted in terms of weak contact initiation, strong bond arrest, and weak interface repropagation.
- (4) SEM-EDS observations provide qualitative microstructural support for the proposed crack propagation mechanism. Si bearing phase rich regions remain relatively intact and can inhibit crack propagation to some extent. Cracks are more likely to propagate along interfaces where Si bearing and Fe bearing phases are intergrown, showing that heterogeneous mineral interfaces are important pathways for crack coalescence. Fe bearing phase rich regions do not necessarily develop through going internal cracks; their failure is still controlled by local weak interfaces and mineral boundaries. Overall, the Fe3O4/SiO2 ratio controls the non monotonic strength variation and macroscopic failure mode by modifying the load bearing framework and weak interface network.
Acknowledgments
The authors thank the PFC development team for providing the software used in the numerical simulations of this study. Methods: Ethics declaration statement: The authors confirm that this work is original, has not been published elsewhere, and is not under simultaneous consideration by any other journal. The research has been conducted with integrity, without fabrication, falsification, or plagiarism. All sources have been properly acknowledged, and the manuscript has been prepared in accordance with the journal’s ethical standards. All authors have approved the submission.
References
- 1. Du K, Sun Y, Zhou J, Khandelwal M, Gong F. Mineral composition and grain size effects on the fracture and Acoustic Emission (AE) characteristics of rocks under compressive and tensile stress. Rock Mech Rock Eng. 2022;55(10):6445–74.
- 2. Zhang Q, Ma R, Lin P, Xie H, Wang Z, Kang J, et al. The influence of mineral composition on uniaxial compression mechanical properties of granite based on PFC-GBM method. J Shandong Univ (Eng Sci). 2025;55(4):93–107.
- 3. He C, Wang X, Shi Q, Zhao G, Li W, Mishra B. 3D analysis of mineralogical and fracture features in granite and impact of biotite distribution on uniaxial compressive strength. Eng Geol. 2025;356:108279.
- 4. Zhou Y, Lv W, Li B, Liang Q. Impact of soft minerals on crack propagation in crystalline rocks under uniaxial compression: A grain‐based numerical investigation. Num Anal Meth Geomech. 2024;48(8):2020–42.
- 5. Hu X, Xie N, Zhu Q, Chen L, Li P. Modeling damage evolution in heterogeneous granite using digital image-based grain-based model. Rock Mech Rock Eng. 2020;53(11):4925–45.
- 6. Zhang S, Qiu S, Kou P, Li S, Li P, Yan S. Investigation of damage evolution in heterogeneous rock based on the grain-based finite-discrete element model. Materials (Basel). 2021;14(14):3969. pmid:34300883
- 7. Liu G, Chen Y, Du X, Wang S, Fernández-Steeger TM. Evolutionary analysis of heterogeneous granite microcracks based on digital image processing in grain-block model. Materials (Basel). 2022;15(5):1941. pmid:35269172
- 8. Caulk RA. Modeling acoustic emissions in heterogeneous rocks during tensile fracture with the Discrete Element Method. Open Geomechanics. 2020;2:1–19.
- 9. Liu X, Han M, He W, Li X, Chen D. A new b value estimation method in rock acoustic emission testing. JGR Solid Earth. 2020;125(12).
- 10. Ma J, Wu S, Zhang X-P, Gan Y. Modeling acoustic emission in the Brazilian test using moment tensor inversion. Comp Geotech. 2020;123:103567.
- 11. Jing G, Wang S, Zhao L, Dong F, Fan Y. Numerical simulation of crack propagation and AE precursor characteristics in coal failure under confining pressures. Sci Rep. 2025;15(1):22750. pmid:40595252
- 12. Ma W, Wang J, Li X, Wang T. Crack evolution and acoustic emission characteristics of rock specimens containing random joints under uniaxial compression. Acta Geophys. 2021;69(6):2427–41.
- 13. Zhang X, Sun J, Chen Y, Wang C, Wang C, Ren W, et al. Experimental study on the effects of rock mineral composition and loading rates on the acoustic emission and fracture characteristics in roof strata tensile fracture. Front Earth Sci. 2024;12.
- 14. Aboayanah KR, Abdelaziz A, Haile BF, Zhao Q, Grasselli G. Evaluation of damage stress thresholds and mechanical properties of granite: New insights from digital image correlation and GB-FDEM. Rock Mech Rock Eng. 2024;57(7):4679–706. pmid:39006378
- 15. Jiang X-Y, Wu D, Zhao Z-X, Yang Y, Tian J-W, Wang F-L. Experimental and numerical study on the damage evolution and acoustic emission multi-parameter responses of single flaw sandstone under uniaxial compression. Theoretical and Appl Fracture Mech. 2024;133:104535.
- 16. Zhang J, Che H, Zhang H. Rock crack evolution and acoustic emission characteristics considering crack penetration based on PFC. Chinese J Underground Space and Eng. 2025;21(3):845–53.
- 17. Zhang Y, Shao Z, Wei W, Qiao R. PFC simulation of crack evolution and energy conversion during basalt failure process. J Geophy Eng. 2019;16(3):639–51.
- 18. Ma H, Xu L, Yuan H, Chen F, Liu Z, Zhou L, et al. A review of the discrete element method (DEM) simulation of mineral comminution processes: Part I. Theoretical developments. MetaResource. 2025;2(4):257–83.
- 19. Nikolaeva NV, Aleksandrova TN, Chanturiya EL, Afanasova A. Mineral and technological features of magnetite-hematite ores and their influence on the choice of processing technology. ACS Omega. 2021;6(13):9077–85. pmid:33842777
- 20. Tian H, Zhu D, Pan J, Yang C, Huang W, Chu M. Effect mechanism of aluminum occurrence and content on the induration characteristics of iron ore pellets. Int J Miner Metall Mater. 2023;30(12):2334–46.
- 21. Pan J, Tang C, Yang C, Zhu D, Guo Z, Huang W. Effect of alumina occurrence form on metallurgical properties of hematite and magnetite pellets. J Iron Steel Res Int. 2023;31(4):797–809.
- 22. Purohit S, Pownceby MI, Guiraud A. Sticking and swelling of iron ore pellets: Mechanisms and controlling factors. J Sustain Metall. 2025;11(1):67–87.
- 23. Basha SM, Biswas P, Dwarapudi S, Misra S, Kamaraj A. Mineralogical characterization and thermal behavior of high-alumina iron ore fines. J Sustain Metall. 2026;12(2):2318–35.
- 24. Prasad R, Soren S, Kumaraswamidhas LA, Pandey C, Pan SK. Experimental Investigation of different fineness and firing temperatures on pellets properties of different iron ore fines from Indian mines. Materials (Basel). 2022;15(12):4220. pmid:35744283
- 25. Cheng S, Hayes PC, Jak E. Iron ore sinter macro- and micro-structures, and their relationships to breakage characteristics. Minerals. 2022;12(5):631.
- 26. Nshimiyimana C, Chisakulo E, Nsengiyumva C. Occurrence and lithogeochemical composition of iron ore in Ngororero District, Rwanda. Heliyon. 2024;10(10):e31319. pmid:38813223
- 27. Zeng Z, Zhang D, Han P, Chang Y, Zhang W, Xu J, et al. A review of microseismic source location techniques in underground mining. MetaResource. 2025;2(3):157–81.
- 28. Hazzard JF, Collins DS, Pettitt WS, Young RP. Simulation of unstable fault slip in granite using a bonded-particle model. Pure appl geophys. 2002;159(1):221–45.
- 29. Knopoff L, Randall MJ. The compensated linear-vector dipole: A possible mechanism for deep earthquakes. J Geophys Res. 1970;75(26):4957–63.
- 30. Vavryčuk V. Moment tensor decompositions revisited. J Seismol. 2014;19(1):231–52.
- 31. Feignier B, Young RP. Moment tensor inversion of induced microseisnmic events: Evidence of non‐shear failures in the −4 < M < −2 moment magnitude range. Geophy Res Letters. 1992;19(14):1503–6.
- 32. Zhao Y, Yang T, Zhang P, Xu H, Wang S. Inversion of seepage channels based on mining-induced microseismic data. Int J Rock Mech Mining Sci. 2020;126:104180.
- 33. He C, Mishra B, Shi Q, Zhao Y, Lin D, Wang X. Correlations between mineral composition and mechanical properties of granite using digital image processing and discrete element method. Int J Mining Sci Tech. 2023;33(8):949–62.
- 34. Niu S, Wu J, Chen S, Zhao J. Investigation of fracture properties of mode I fracture in heat-treated granite. Sci Rep. 2025;15(1):13679. pmid:40259002
- 35. Liu K, Zhao J. Progressive damage behaviours of triaxially confined rocks under multiple dynamic loads. Rock Mech Rock Eng. 2021;54(6):3327–58.
- 36. Wang S, Zhou J, Zhang L, Han Z, Zhang F. Parameter studies on the mineral boundary strength influencing the fracturing of the crystalline rock based on a novel Grain-Based Model. Eng Fract Mech. 2021;241:107388.
- 37. Wong LNY, Peng J, Teh CI. Numerical investigation of mineralogical composition effect on strength and micro-cracking behavior of crystalline rocks. J Natural Gas Sci Eng. 2018;53:191–203.
- 38. Hofmann H, Babadagli T, Yoon JS, Zang A, Zimmermann G. A grain based modeling study of mineralogical factors affecting strength, elastic behavior and micro fracture development during compression tests in granites. Eng Fracture Mech. 2015;147:261–75.
- 39. Zhang L, Zhou J, Peng X, Zhang L-Q, Li X, Wang S, et al. Contact heterogeneity control on fracture and acoustic emission evolution in granite: Evidence from PFC3D-GBM and AE–MT inversion. Eng Fracture Mech. 2026;343:112323.
- 40. Zhao X, Wang Z, Pan P-Z, Xie Y, Yang N, Yu P, et al. Experimentally informed grain based modelling of asynchronous mineral scale fracturing in heterogeneous granite. Eng Fracture Mech. 2026;340:112140.
- 41. Tan Y, Zeng Z, Yang J, Liu J, Song W. Review on macro-meso mechanical properties and damage mechanism of rock-backfill composite structure. MetaResource. 2026;3(2):213–40.
- 42. Liang J, Jin C, Li G, wang Q. Instability mechanisms and collapse range prediction of steep high slopes during the open-pit to underground transition: A case study. Eng Geol. 2026;365:108625.
- 43. Li J, Liu Y, Yang T, Xu T, Liu F, Li G, et al. Shear-creep-induced strength degradation of soft–hard interbedded rock masses controlled by layer-thickness ratio: Implications for progressive failure of anti-dip slopes. Int J Rock Mech Mining Sci. 2026;208:106745.
- 44. Li J, Yang T, Deng W, Du S, Zhang Z, Ma H, et al. Evaluating failure mechanisms of excavation-induced large-scale landslides in Xinjing open-pit coal mine through integrated UAV imagery and 3D simulation. Landslides. 2025;22(6):2021–36.

관련 뉴스