Electrical, mechanical, and morphological properties of nano-filled HTV-SR/EPDM blends under AC corona aging
Figures
Abstract
Among the various factors, corona discharge is recognized as one of the most threatening to degrade polymeric insulators. Over time, corona-induced deterioration has become a more dominant phenomenon in extra- and ultrahigh-voltage transmission lines. Therefore, this study investigates the aging effects on optimally balanced weight-percentage samples of high-temperature-vulcanized silicone rubber/ethylene-propylene-diene monomer (HTV-SR/EPDM) incorporating boron nitride (BN) and silicon carbide (SiC) fillers to identify the most desirable composition for resistance to degradation. The nano-sized fillers were loaded at 1, 3, and 5 wt.%. The test samples were subjected to an AC corona discharge for 72 h, utilizing a multi-needle high-voltage electrode and a plane-grounded electrode arrangement. The deterioration characteristics of the blend materials, both before and after aging, were evaluated through electrical, morphological, and mechanical analyses encompassing volume conductivity, dielectric response, scanning electron microscopy, tensile strength, and hardness measurements. The results revealed that at 8 kV stress across 30–60 °C, corona exposure increased the volume conductivity of 3 wt.% BN nanocomposites by only 25.8%–36.5%, whereas the unfilled blend experienced a much higher increase of 45.3%–88.3%. After corona exposure, high-loading nanocomposites retained up to 42.4% greater tensile strength than the degraded unfilled blend. The surface roughness was relatively lower for the filled blend samples following the corona discharge. Overall, the blend sample with 3 wt.% of BN demonstrated consistent behavior under all investigated conditions, indicating better corona-aging retardation. It has been shown that the incorporation of nano-sized fillers retards material degradation, thereby enhancing the performance of polymeric insulation.
Citation: Saleem MZ, Noorden ZA, Yiew LK, Salem AA, Algamili AS (2026) Electrical, mechanical, and morphological properties of nano-filled HTV-SR/EPDM blends under AC corona aging. PLoS One 21(11): e0363673. https://doi.org/10.1371/journal.pone.0363673
Editor: Karthik Kannan, National Chung Cheng University College of Engineering, TAIWAN
Received: August 9, 2026; Accepted: November 10, 2026; Published: November 24, 2026
Copyright: © 2026 Saleem et al. This is an open access article distributed under the terms of the Creative Commons Attribution License, which permits unrestricted use, distribution, and reproduction in any medium, provided the original author and source are credited.
Data Availability: The data supporting the findings of this study are entirely presented within the figures, tables, and text of the paper. No external or additional datasets were generated or required.
Funding: The author(s) received no specific funding for this work.
Competing interests: The authors have declared that no competing interests exist.
Introduction
The increased voltage levels of electrical transmission networks demand a more sophisticated outdoor insulation system to meet the growing power demand. In transmission systems, where lines operate at extra- and ultra- high-voltages, the insulation experiences severe stress from electrical, mechanical, and environmental conditions, causing more dominant corona-induced discharges [1,2]. These discharges produce ozone and deposit ions on surfaces, and may also cause cracks and formation of hydrophilic groups (OH) due to the oxidation of methyl and hydrocarbon groups, which serve as insulation failure precursors [2]. In long-term service, this behavior strongly affects the hydrophobicity of insulating material, contributing to severe surface aging and eventual puncturing of the sheds [3]. Among polymeric materials, silicone rubber (SR), ethylene-propylene-diene monomer (EPDM), and epoxy resins are the most commonly employed for manufacturing polymeric insulating weather sheds to potentially substitute conventional glass and porcelain insulators [3–6]. Polymeric insulators offer the advantages of being lightweight, easy to handle during transportation and maintenance, low-cost to install, and superior pollution performance owing to their high hydrophobicity [7,8]. However, electrical and environmental stresses may contribute to the deterioration of polymeric materials due to their organic nature [4,9,10]. Therefore, anti-aging requires the selection of suitable insulating materials and their proper diagnosis, particularly of corona discharge aging, to enhance their performance during long-term service in an outdoor environment [11].
Over the past two decades, numerous studies have been conducted to understand the corona-induced modifications of polymers. Researchers in most studies have focused on developing corona discharge test setups using different electrode arrangements [9,12,13], the impact of applied voltage types [14,15], and various aging assessment techniques [16,17]. Among the various arrangements, including flat plate electrode, single-needle plate electrode, and multiple-needle plate electrode, the latter can deteriorate a larger area of the test specimen, thus facilitating the characterization of corona impact through various tests, as recommended by the CIGRE working group D1.14 [1,9]. In corona discharge studies considering voltage types, it was found that AC corona has a greater impact on damaging the material as compared to DC voltage [14]. Furthermore, to enhance the severity of the corona discharge and hence the material aging, the combined impact of electrical (corona discharge) and environmental stresses, such as temperature, humidity, salt fog, and ultraviolet radiation, was investigated in a corona chamber [10,18–21]. After the corona discharge treatment, the degree of deterioration of the studied materials was mostly evaluated using scanning electron microscopy (SEM), Fourier transform infrared (FT-IR) spectroscopy, and contact angle measurements. In recent studies, emerging diagnostic techniques such as atomic force microscopy (AFM), laser-induced breakdown spectroscopy (LIBS), and different machine learning models have been employed to assess material degradation [12,13].
Researchers have investigated the incorporation of different types of inorganic fillers (particularly those with higher thermal conductivity and loadings within the 1 wt.% to 5 wt.% range) in base materials to improve the characteristics of polymer nanocomposites, focusing on reducing the aging caused by corona discharge [2,22–25]. For example, in [22], nano-sized ATH incorporated in silicone rubber was evaluated under water-droplet-initiated surface discharges to retard higher surface roughness and increase the charge trap depth. The measurements indicated that the sample doped with 5 wt.% nano-ATH provides the desired characteristics. Similar work has been conducted on epoxy containing Al2O3 nanoparticles to improve the corona inception voltage and tensile strength [23]. In another study, the corona aging of epoxy samples with different doping contents of nano-Al(OH)3 was examined under environmental stresses of high humidity and high temperature [25]. After corona aging for 100 h under harsh conditions, it was found that adding 3 wt.% of nanofiller to the base polymeric material provides enhanced resistance against aging, particularly its hydrophobicity and surface resistivity. In [26], nano-BN filled in silicone rubber to replace ATH fillers was investigated, and the analysis revealed enhanced breakdown and reduced dielectric loss. Another contribution highlighted the use of BN coating on SiO2 in epoxy material to enhance the thermal conductivity and insulating properties of the composites [27]. Similarly, BN was incorporated into transformer oil to enhance its thermal capability by approximately three times and tensile strength by 35% compared to insulation paper [28].
In conjunction with this literature, which incorporates nanoparticles into a single base matrix, advancements in blending methods have made it possible to incorporate nanofillers and retain the intended electrical and mechanical characteristics of two different base matrices [29–32]. For example, nano-MgO incorporated in a blend of polypropylene (PP)/ethylene-propylene-diene monomer (EPDM) has been examined for use as a high-voltage power cable insulation material [30]. In another study, nanoparticles of nano-silica (SiO2) and nano-titanium dioxide (TiO2) were doped into an SR/EPDM blend to enhance its electrical and mechanical properties [31,32]. However, very limited studies are available in the literature that emphasize the use of nanofillers in blend materials, particularly their contribution to enhancing the aging performance of corona resistance. Moreover, the assessment of volume degradation (through increasing volume current/conductivity and activation energy), especially at higher ambient temperatures and voltage levels, is of particular interest and needs to be investigated at length. This is also practically significant for HV insulation applications, to explore new insulating blend materials with emerging nanoparticles, such as BN and SiC used in this study, to impede their deterioration under AC corona discharge.
Based on the above, the study described herein aims to enhance the resistance of studied materials against corona-induced deterioration in high-voltage outdoor usage. To this end, corona discharge treatment for 72 h of high-temperature-vulcanized silicone rubber/ethylene-propylene-diene monomer (HTV-SR/EPDM) blends containing an optimally balanced weight percentage (50:50 wt.% of HTV-SR/EPDM) and addition of nano-sized contents of boron nitride and silicon carbide was investigated. Following this activity, volume conductivity and dielectric response measurements were used to perform diagnostics on the test samples. In addition, to evaluate the volume conductivity, diagnostic techniques were employed at electric fields ranging from 0.5–4 kV/mm and ambient temperatures of 30 ℃ and 60 ℃. Particularly, the activation energies of the studied samples were compared for volume deterioration. The mechanical properties of all unaged and aged samples were examined by measuring the tensile strength (TS) and hardness, while the morphological effects of aging were assessed using scanning electron microscopy (SEM). The diagnostic techniques and results of this study can provide guidelines for the evaluation of the properties of insulating materials.
Experimental methods
Preparation of HTV-SR/EPDM blends
To fabricate the different blend samples, the base materials used were HTV-SR and EPDM. Two nano-sized particles, namely boron nitride (BN) and silicon carbide (SiC), were separately used as fillers, with detailed specifications listed in Table 1. Di-cumyl peroxide (DCP) was incorporated as a curing agent at 2.5 parts per hundred of rubber (PHR). For the preparation of the blend samples, firstly, HTV-SR and EPDM were mixed in a two-roll mill mixing machine operating at 110 ℃, with the front- and rear-roller fixed at 12.2 rpm and 14.6 rpm, respectively. The required amounts of filler and DCP were then mixed in the blend mixture for 20 min. Thereafter, to cure the blended materials having various quantities of filler, the compound was pressed using a hydraulic electrical hot-press dual heat plates machine set at 10 MPa pressure with a temperature of 180 ℃ for 3 min. Lastly, the samples post-curing was carried out for 2 h at 150 ℃. Finally, the samples were prepared as flat sheets with dimensions of 15 × 11 × 0.2 cm3. The different composition formulations of prepared HTV-SR/EPDM blends without and with nano-sized particles are listed in Table 2.
Corona discharge experimental setup
The experimental test setup to produce AC corona discharge for 72 h is similar to that used earlier [33]. To make this study self-contained, the necessary information is given here. In the given system, high-voltage test transformer has a rating of 30 kV and 30 kVA, and 20 kV was applied to 31 multi-needle stainless-steel high-voltage needles of various lengths, which were positioned for uniform corona exposure at the sample surface, to age the test material [33]. The other electrode holding the test sample was connected to the ground through measurement arrangement for the corona discharge current. The given voltage (20 kV) was chosen with 50 mm gap between the high-voltage and grounded-bottom electrodes, taking into account the following constraints: corona should occur at the applied voltage, and no flashover should occur on the sample. In addition to that, as highlighted in the Introduction section, this arrangement provides a nearly uniform electric field on the sample’s surface to obtain a large uniform degraded area for different investigation techniques after corona treatment. The system, on the other hand, was equipped with foolproof protection in the event of an unintended breakdown or flashover. The corona chamber was made of an acrylic sheet with dimensions of 30 × 30 × 30 cm3 and consisted of a multi-needle and rectangular plate electrode arrangement. For the corona chamber ventilation, a DC (12 V) air compressor pump with an airflow of 5 L/min was employed to reduce the potential influence of ozone. During the experiment, temperature and humidity levels were monitored, and these were recorded as (18–22 ℃) and 55 ± 10%, respectively. Fig 1 illustrates the discharge current pulses recorded for one min on one test sample using a PicoScope during AC corona discharge.
Diagnostic measurement of HTV-SR/EPDM blends filled with nanofillers
Volume current measurement.
To assess the impact of corona discharge on the volume current of the blend samples, the experimental arrangement for measuring this electrical characterization is portrayed in Fig 2. Moreover, a three-electrode arrangement was used to hold and energize the test specimen, which is based on the ASTM D257 standard. The three electrodes are referred to as high voltage (HV), measuring, and guard (in the shape of a ring) connected to the ground. The volume current is measured across the test sample. A Glassman (model FJ20P6) HV source was used to generate a DC voltage ranging from 0 to 20 kV and connected to an HV electrode. To account for equipment measurement uncertainty, the voltage output accuracy was maintained within ± (0.5% of setting + 0.2% of rated voltage). A Keysight electrometer (B2981A), providing a minimum current measurement resolution of 0.01 fA and measurement accuracy of up to ±0.05%, connected to a measuring electrode, was used to measure a highly sensitive current (from 0.01 fA to 20 mA) across the test specimen. The test system included protection to protect the electrometer in the event of a flashover across the sample surface. The real-time current was measured and recorded using the LabVIEW software.
The three-electrode system with the inserted sample was placed inside an oven with grounded metallic walls to avoid external electromagnetic disturbances and maintain isothermal conditions. The temperature dependence of the volume current was recorded at 30 and 60 °C. Prior to energizing the test specimen, the test temperature was set to the desired value. A DC voltage of 1 kV was then applied for a time span to reach the current at a nearly steady-state value. Subsequently, the voltage was raised to the next step to measure the current at 3–8 kV, and field dependence of the current was evaluated. To ensure that the measurement was free from residual polarization, the sample was grounded and short-circuited after each experiment. The presented data are mean values of at least three different experiments. Variation of results (found to be less than ±10%) is not shown intentionally, as the figures are already quite dense with information.
First, the bulk resistance () of the material was determined by applying a voltage potential (V) and measuring the resulting steady-state current (Iv) flowing through the volume/bulk of specimen using equation(1). Then, the volume/bulk conductivity of the specimen was calculated through equation (2), which used and dimensions of the measuring electrode from a standardized three-electrode system.
(1)(2)Here, the volume/bulk conductivity of the specimen is denoted by , and S is the surface area of the measuring electrode with an effective electrode size of 0.002734 m2. The material thickness in the direction of the electric field is denoted by H.
The temperature dependence of volume conductivity was further described using the Arrhenius expression given in equation (3).
(3)Here, represents the volume conductivity at an ambient temperature (T). Where, is a constant, R is the constant, and the activation energy is denoted by .
Dielectric response measurement
Corona discharge activity generates high-frequency signals and may influence both the real and imaginary permittivities, as well as the dielectric loss of an insulating material [34]. To investigate the studied test samples for such effects, the dielectric response characteristics of the materials before and after exposure to corona discharges were measured using a precision impedance analyzer micro-test 6630−5, featuring a basic measurement accuracy of ±0.05% and a frequency output accuracy of ±0.01%. This instrument was equipped with an in-built electrode cell (component fixture FX-0000C6) for holding the test sample. Measurements were performed at ambient room temperature in the frequency range of 10 Hz to 1 MHz. For each sample, both the complex permittivity (consisting of real and imaginary parts) and dielectric loss factor were recorded. Reported data represent the mean of at least three measurements; error bars are omitted to preserve figure clarity.
Scanning electron microscopy (SEM) analysis
To assess the uniformity of distribution of filler particles in the base blend of HTV-SR and EPDM, analysis was performed using a Zeiss EVO 15 (SEM). Moreover, post-corona-aged surface morphological changes of the test samples were analyzed. The test procedure involved sputter-coating the test specimen under investigation with a copper layer of 2 nm prior to capturing the SEM image. This step was taken as a precautionary measure against charge deposition on the sample surface due to bombardment by the electron beam.
Mechanical properties
In addition to the insulating and physicochemical properties, mechanical characteristics are essential for the reliable operation of insulators. The long-term reliable operation of polymeric insulators in outdoor applications requires the retention of their mechanical integrity under environmental constraints. Therefore, an attempt was made to study the mechanical properties of the test samples to evaluate the effect of corona discharge. The mechanical properties of unaged and corona-aged samples were assessed by measuring the tensile strength (TS) and hardness. The samples were cut into dumbbell shapes to perform a tensile strength test under a strain rate of 10 mm/min using a universal testing machine (Instron 5567) with a 30 kN load capacity and position resolution of 6.1 µm. The samples were prepared with gauge dimensions of 5 mm in width and 22 mm in length according to the standards (ASTM D638), and the tensile strength was recorded based on equation (4) [35]. Three test samples of each composition were tested to verify repeatability, and the average value was recorded.
(4)Here, is the tensile force at sample break, D represents the gauge width, and the material thickness is denoted by H.
Likewise, the hardness of different samples before and after corona discharge was measured by employing a Shore-A durometer, and these measurements were performed according to the ASTM D2240 standard guidelines [36]. The recorded value was the average of three readings taken from different points on each sample.
Results and discussion
Volume current
Fig 3 shows the recorded volume current of three different blend samples at voltage levels of 1–8 kV and ambient temperatures of 30 ℃ and 60 ℃. As can be seen, each spike/peak in the time-varying current data indicates the capacitive current, resulting from varying the voltage from 1 to 8 kV in steps of 3 kV, 5 kV, and 7 kV. Then, it starts to stabilize following a slowly decaying polarization process to give a steady-state conduction current in the test material at a given applied voltage. This final value of current is further utilized in equation (2) to calculate the volume conductivity of the test material. Table 3 provides the volume conductivity of all unaged and corona-aged test samples at two voltage levels and ambient temperatures of 30 ℃ and 60 ℃. For comparison, the conductivity values are provided in the same column, as a ratio (numerator for unaged and denominator for aged samples), for a specific voltage and ambient temperature. It was observed that incorporating the nanofiller lowered the volume current and, hence, the deduced volume conductivity. For instance, in unaged samples, at a fixed ambient temperature (30 ℃) and at two voltage levels of 1 kV and 8 kV, the volume conductivity for all filled samples is lower as compared to the unfilled sample (B0). The same was true for all investigated samples at higher ambient temperatures. In general, nanofillers at higher concentrations lower the volume conductivity by more than one order of magnitude. In the unaged samples, among the different fillers as well as their concentrations, the volume conductivity was lowest for the blend sample filled with 3 wt.% of BN as compared to 3 wt.% of SiC. This behavior is attributed to the insulating nature of BN particles [24]. But, at high concentration (5 wt.%), the volume conductivity of blend sample B3 started to increase instead of decreasing. This behaviour can be explained by the inter-particle spacing calculated using Tanaka’s model [37]. As filler loading increases, the inter-particle spacing systematically decreases, reaching minimum values of 53.65 nm for and 65.99 nm for B6. As the inter-particle distance approaches the average nanoparticle size (50 nm), the adjacent interaction zones surrounding the nanoparticles begin to overlap [38]. This forms continuous conductive channels, thereby enhancing volume conduction despite the higher filler content. However, the value of conductivity at the highest concentration is still low compared to that of the unfilled blend sample. Overall, it can be seen that the volume conductivity increases in both unaged and corona-aged test materials, either by increasing the voltage level or ambient temperature.
The current spikes in the data of each sample appeared at 1, 3, 5, 7, and 8 kV.
To quantify the impact of applied voltage and ambient temperature on material aging and the overlapping mechanism, the plot of activation energy, calculated from the results of natural logarithm of volume conductivity, versus the reciprocal of temperature for three samples (B0, B2, and B5) is shown in Fig 4. The data points were linearly fitted, indicating though slope of solid and dotted lines, for applied voltages of 1 and 8 kV. The results were obtained for both unaged and corona-aged samples (see Fig 5). The results indicated that the activation energy differs after the incorporation of different types of nanofillers into the blend material. The activation energy for BN-filled samples was comparatively higher as compared to SiC-filled samples. At 1 kV, before and after corona exposure, the change in activation energy for all studied materials was not significant. After corona discharge, this decrease in the activation energy was minimum for blend B2 as shown in Fig 4(b). Furthermore, a negligible change in activation energy was observed in blend B2 compared to that in B5 at high temperature, even after corona exposure, indicating less degradation owing to better resistance offered by the BN particles. The activation energy was lowest for sample B3 among the BN-filled materials, which may be attributed to poor nanofiller dispersion and localized agglomeration. However, at a higher temperature of 60 ℃ and an applied constant voltage of 8 kV, the activation energy increases, particularly for samples B0, B2, and B5; but this increase is more prominent in the unfilled sample after corona exposure. This behavior indicates that even though the activation energy is highest for B0, the applied field becomes more significant in overcoming the thermal barriers and allowing conduction after the corona discharge.
The activation energy was extracted from the slope of the linear fit of the data points.
Note that * and ^ represent the calculated value for the test sample before and after corona discharge, respectively.
Dielectric spectroscopy
Frequency dependence of the real () and imaginary () parts of the complex permittivity of the studied materials are shown in Figs 6 and 7, respectively. Data recorded both prior to and after corona-aging are displayed. As shown, the is approximately constant in the frequency spectrum ranging from 103 to 106 Hz. Although, its value is different depending on the material’s composition, being higher for the additionally filled blends as compared to the unfilled sample B0. Moreover, a small increase can also be noticed at lower frequencies, which may be attributed to the interfacial polarization between the filler particles (particularly in the materials additionally doped with nano-sized BN and SiC) and the base matrix [22]. It is worth highlighting that material samples are always reinforced with some fillers, for instance, for mechanical strength, apart from the additional fillers that are incorporated for achieving other specific requirements. The influence of SiC filler on elevating the real permittivity of the studied test samples was slightly higher than compared to BN. Furthermore, aging the materials under corona discharge also uplifted their , although insignificantly, as demonstrated in Fig 6(b).
To assess how the corona discharge affects dielectric loss, imaginary permittivity of the test samples, shown in Fig 7(b), was analyzed. For comparison, the values measured prior to corona-aging are also displayed in Fig 7(a). Moreover, for quantifying the severity of aging, the dielectric loss factor calculated at three different frequencies is listed in Table 4. Examining these results, it can be argued that varies by two orders of magnitude within the studied frequency range. The higher values on the left, where frequency is relatively low, may be associated likewise real permittivity, with the increasing effect of interfacial polarization or Maxwell Wagner-Sillars, as reported in [22]. Similarly, aging the investigated blends also elevated the losses, although, the difference between the pre- and post-aged data is rather weak, as demonstrated by both the figures and tabulated values.
SEM
SEM images of various test samples taken before and after exposure to the corona discharge at a magnification level of 500 are displayed in Fig 8. The presented data show a fairly smooth surface for the studied samples in their unaged condition. Even though, for relatively heavily doped samples, only a moderate level of surface roughness can be noticed, particularly for HTV-SR/EPDM filled with 3 wt.% of SiC. On the other hand, post-corona aging data exhibited noticeable surface degradation of the test samples, showing a dependence on their composition. The relatively high concentration of nano-sized BN filler seems to be non-uniformly dispersed in the base matrix, as evident from the white spots on the surface of B3 sample. This is known as an agglomeration phenomenon, which has been reported [10]. Irregularities of this kind may cause surface unevenness and fragmentation, leading to high surface roughness. Nevertheless, corona-induced damage of the studied blends B2 and B5, incorporated with additional fillers, is relatively small compared to sample B0. Under corona discharge, high-energy electron impacts and reactive radical species readily cleave the hydrophobic Si-O-Si and C-C backbones in the unfilled polymer matrix [1,16]. In contrast, the incorporated nanoparticles, particularly BN, possess high intrinsic bond strength and superior thermal dissipation capabilities [24,26]. They act as localized micro-thermal sinks that rapidly conduct heat away from discharge sites, thereby mitigating thermal oxidation and reducing main-chain scission. This thermal shielding effect effectively hinders severe surface erosion, pitting, and micro-cracking under electrical stress [12].
Sub-figures (a), (b), (c), and (d) show images of the unaged test samples B0, B2, B3, and B5, respectively, while (e), (f), (g), and (h) represent images after their exposure to corona discharge.
Mechanical properties
It has been observed from the electrical properties of all investigated samples that the blend samples had a less damaging effect as compared to the unfilled sample. Based on this observation, the tensile strength and hardness of blend materials were measured before and after corona aging to investigate their mechanical integrity. Table 5 lists the average values of these two parameters. The tensile strength continued to increase with increasing filler concentration, indicating better interface interaction between the base matrix and nanofiller [39]. For example, the highest tensile strength values of 4.07 MPa and 4.11 MPa were achieved for samples B3 and B6, respectively. Similarly, as can be seen, the hardness of blend materials increased with the loading of BN nanofillers. However, a slight reduction in hardness was observed after corona exposure. A similar trend was observed for the SiC-filled samples. These reductions are not considered significant and cannot cause mechanical failure of samples after 72 h of corona discharge.
Conclusion
This study was carried out not only to demonstrate how materials degrade when subjected to corona discharge, but also to determine the composition of materials that resist this impact, thereby improving the performance of insulating systems in outdoor high-voltage applications. In this context, the insulation characteristics of studied materials before and after uninterrupted corona exposure for 72 h were assessed by measuring their electrical, dielectric, physicochemical, and mechanical properties. The acquired results indicated that the BN nanofiller imparts better resistance to volume current at lower concentrations (for example at 3 wt.%) under the prevailing conditions of higher voltage levels and ambient temperatures. Although a slight reduction in surface roughness was observed in nano-filled blended samples, it helped enhance the barrier resistance, which impedes damage to the organic structure. Moreover, the incorporation of nanofillers improved the mechanical properties of the two base materials, while corona exposure had the least influence on reducing tensile strength. According to the collected data, BN-doped materials outperformed their SiC-filled equivalents, with the most promising composition being 97 and 3 wt.% of HTV-SR/EPDM blend and nano-sized filler, respectively. Further research can be undertaken by considering the hybrid composition of the most commonly employed fillers, such as silica, aluminum trihydride, and boron nitride. In addition, studies on long-term corona severity should consider employing environmental parameters, such as humidity, UV, and temperature.
Acknowledgments
The authors would like to acknowledge the support provided by Universiti Teknologi Malaysia (UTM) under the UTM Flagship CoE/RG and Professional Development Research University Special Research programs. The authors also gratefully acknowledge the multifaceted support provided by the Ghulam Ishaq Khan Institute of Engineering Sciences and Technology (GIKI) in conducting this research.
References
- 1. Bi M, Deng R, Jiang T, Chen X, Pan A, Zhu L. Study on Corona Aging Characteristics of Silicone Rubber Material under Different Environmental Conditions. IEEE Trans Dielect Electr Insul. 2022;:1–1.
- 2. Kavitha N, Dhivakar JM, Bhavani NPG, Sarathi R, Kornhuber S. Understanding the impact of different nanofillers on electrical, thermal, and surface properties of corona-aged silicone rubber nanocomposites. Polym Compos. 2025;46:1686–98.
- 3. Zeng S, Li W, Zhao X, Peng Y, Liu Y, Yan X, et al. Lifespan Evaluation of HTV Silicone Rubber in Outdoor Composite Insulators Considering Temperature Cycling and Corona Discharge. IEEE Trans Dielect Electr Insul. 2025;32(4):2403–12.
- 4. Rehman AU, Khan MS, Rashid A, Khattak A, Khan A. Electro-UV and electro-thermal aging effects on the electrical and surface properties of HTV silicon rubber nanocomposites for electrical insulation. Silicon. 2026;:1–17.
- 5. Bi M, Rao X, Wen Y, Peng H, Jiang T, Tang J. Study on Corona Aging Characteristics of Epoxy Resin Under Different Hygrothermal Environments. IEEE Trans Dielect Electr Insul. 2023;30(5):2249–57.
- 6. Rihan M, Ahmed Z, Nasrat LS. Advancing High-Voltage Polymeric Insulators: A Comprehensive Review on the Impact of Nanotechnology on Material Properties. SVU-International Journal of Engineering Sciences and Applications. 2025;6(1):93–105.
- 7. Tan DQ. The search for enhanced dielectric strength of polymer-based dielectrics: A focused review on polymer nanocomposites. J Appl Polym Sci. 2020;137:1–32.
- 8. Rehman AU, Khan MS, Rashid A, Khattak A, Imran K, Kazmi SAA. Failure analysis of HTV silicone rubber/ZnO nanocomposites: synergistic electro-UV and electro-thermal aging effects. Eng Fail Anal. 2026;110893.
- 9. Bi M, Qiu R, Duan S, Deng R, Xi C, Jiang T. Effects of Hygrothermal Conditions on Corona Aging of Silicone Rubber. IEEE Trans Dielect Electr Insul. 2025;32(2):992–1000.
- 10. Banerjee S, Prasad DS. AC Corona Degradation of Silicone Rubber Nanocomposites at Low Air Pressure. IEEE Trans Dielect Electr Insul. 2022;29(3):800–7.
- 11. Saleem MZ, Akbar M. Review of the Performance of High-Voltage Composite Insulators. Polymers (Basel). 2022;14(3):431. pmid:35160421
- 12. Nazir MT, Phung BT, Yu S, Abbas G, Abid M, Wang C. Resistance against AC corona discharge of micro-ATH/nano-Al2O3 co-filled silicone rubber composites. IEEE Transactions on Dielectrics and Electrical Insulation. 2018;25:657–67.
- 13. Tahir MH, Arshad A, Manzoor HU. Influence of corona discharge on the hydrophobic behaviour of nano/micro filler based silicone rubber insulators. Mater Res Express. 2022;9(3):035302.
- 14. Krupanandam G, Dhivakar JM, Kornhuber S, Sarathi R. Understanding the dielectric properties of silicone rubber BN nanocomposites under DC voltage. Polym Eng Sci. 2024;65:732–44.
- 15. Ibrahim Uckol H, Ilhan S. Corona Discharge Modes and Their Detections Under DC and AC Voltages. IEEE Sensors J. 2024;24(10):17019–26.
- 16. Thangabalan B, Neelmani VNJ, Sarathi R, Harid N, Griffiths H. Understanding the Surface Condition of Silicone Rubber Nanocomposite Due to Corona Aging Using AFM Imaging and LIBS Spectroscopy. IEEE Trans Dielect Electr Insul. 2022;29(6):2089–100.
- 17. Manoj Dhivakar J, Prawin K, Jayaganthan R, Tiwari S, Kornhuber S, Sarathi R. Thermography and Machine Learning Analysis of Corona Aging of Silicone Rubber Nanocomposites. IEEE Trans Dielect Electr Insul. 2025;32(1):263–72.
- 18. Mahmood A, Muneeb A, Saeed U, Alam S, Al-Ammar EA, Kang JH, et al. Aging assessment of silicone rubber materials under corona discharge accompanied by humidity and UV radiation. Nanotechnol Rev. 2024;13:20240018.
- 19. Belhiteche EH, Rondot S, Moudoud M, Dony P, Jbara O. Electrical insulation properties of silicone rubber under accelerated corona and thermal aging. Polym Eng Sci. 2020;60:1–10.
- 20. Lu M, Zeng S, Gao C, Liu Y, Yan X, Liu Z, et al. Aging Analysis of HTV Silicone Rubber Under Coupled Corona Discharge, Humidity and Cyclic Thermal Conditions. Electronics. 2025;14(20):4071.
- 21. Qiao X, Shi R, Ye W, Zeng W, Zhao J, Zhang J. Early surface powdering phenomenon and formation mechanism of silicone rubber sheaths for UHV bushings under corona-dominated multi-factor aging. Electric Power Systems Research. 2026;258:113114.
- 22. Manoj Dhivakar J, Sarathi R, Kornhuber S. Investigation on Electrical, Thermal, and Mechanical Properties of Silicone Rubber ATH Nanocomposites. IEEE Access. 2022;10:94040–50.
- 23. Neelmani SR, Suematsu H, Tanaka T. Influence of nanofiller dispersion on electrical and mechanical properties of epoxy alumina nanocomposites. Res Compos Mater Appl. 2021;31:223–35.
- 24. Ganesan K, Dhivakar JM, Kornhuber S, Sarathi R, Danikas MG. Investigation on the role of interface on electrical, thermal and mechanical properties of silicone rubber BN nanocomposites. J Eng Sci Technol Rev. 2024;17(4).
- 25. Bi M, Du Y, Rao X, Lei S, Chen X, Jiang T. Study on the corona aging characteristics of KH570 modified nano Al(OH)3 cycloaliphatic epoxy resin in hygrothermal environments. Mater Chem Phys. 2025;332:130190.
- 26. Chen X, Wang J, Zhang C, Yang W, Lin J, Bian X, et al. Performance of silicone rubber composites using boron nitride to replace alumina tri‐hydrate. High Voltage. 2020;6(3):480–6.
- 27. Liang T, Guo L. Synergetic enhancement of thermal conductivity and electrical insulating properties in the hexagonal boron nitride coated on silica (SiO2@BN)/BN/Epoxy composites. J Phys Conf Ser. 2025;3006:012032.
- 28. Xu Y, Soori T, Zhang Q, Zhu JY, Nelson JK, Hu L, et al. Boron nitride enhanced electric insulation paper for extending transformer thermal life. Mater Des. 2025;232:114112.
- 29. Li J, Gao Y, Song Z, Liu B, Guo C, Chen Y, et al. Study on thermal cycling ageing resistance of performances of polypropylene/elastomer/boron nitride nanocomposites for high voltage direct current cable insulation. High Voltage. 2024;9(3):556–65.
- 30. Sharip MRM, Lau KY, Noorden ZA, Tan CW, Zaidel DNA, Ching KY. Effects of surface-treated nanomagnesia on the electro-mechanical properties of polypropylene/ethylene-propylene-diene monomer blends. Polym Adv Technol. 2025;36:e70121.
- 31. Vijayalakshmi S, Deepalaxmi R, Rajini V. Electromechanical characterization of titanium-dioxide-filled SiR-EPDM blends. Polym Polym Compos. 2021;29:311–22.
- 32. Alber A, Nasrat L, Ismail H, Hassan M. Electromechanical characterisation of nano silica filled EPDM SiR composite for high voltage insulation. Int J Adv Technol Eng Explor. 2022;9:1610–27.
- 33. Saleem MZ, Akbar M, Alam S. Aging Assessment of Corona-Exposed HTV-SiR/EPDM Blends Loaded With Nanofillers. IEEE Trans Plasma Sci. 2021;49(12):3897–906.
- 34. Hakami MA. Effects of corona discharges on silicone rubber samples under severe environmental conditions. Ontario, Canada: University of Waterloo. 2021.
- 35.
ASTM D638-22: Standard test method for tensile properties of plastics. West Conshohocken (PA): ASTM International. 2022.
- 36.
ASTM International. ASTM D2240-15/21: Standard test method for rubber property—durometer hardness.
- 37. Tanaka T, Kozako M, Fuse N, Ohki Y. Proposal of a multi-core model for polymer nanocomposite dielectrics. IEEE Trans Dielect Electr Insul. 2005;12(4):669–81.
- 38. Liu P, Li L, Wang L, Huang T, Yao Y, Xu W. Effects of 2D boron nitride (BN) nanoplates filler on the thermal, electrical, mechanical and dielectric properties of high temperature vulcanized silicone rubber for composite insulators. Journal of Alloys and Compounds. 2019;774:396–404.
- 39. Ganesan K, Dhivakar JM, Kornhuber S, Sarathi R, Danikas MG. Investigation on the role of interface on electrical, thermal and mechanical properties of silicone rubber-BN nanocomposites. J Eng Sci Technol Rev. 2024;17:16–22.